GR5 Titanium Bar (Ti-6Al-4V) - Product Introduction
Overview
GR5 titanium bar (Grade 5, Chinese designation TC4) is a bar-form product made from the Ti-6Al-4V alloy - the most widely used titanium alloy in the world, accounting for over 50% of total titanium consumption. It combines high strength, low density, excellent corrosion resistance, and good fabricability, making it the standard material for aerospace, medical, marine, and high-performance industrial applications. GR5 bars are typically supplied as hot-rolled, forged, or cold-drawn/ground products with diameters from 3 mm to 300+ mm, in lengths up to 6 meters or as required.
1. Chemical Composition (per ASTM B348 / ASTM F136)
表格
| Element | Content (wt%) | Function |
|---|---|---|
| Titanium (Ti) | Balance (~90%) | Base metal |
| Aluminum (Al) | 5.5 – 6.75% | α-stabilizer; strengthens and improves high-temperature performance |
| Vanadium (V) | 3.5 – 4.5% | β-stabilizer; improves strength, ductility, and hardenability |
| Iron (Fe) | ≤ 0.40% | Impurity limit |
| Oxygen (O) | ≤ 0.20% | Strengthening interstitial (controlled) |
| Carbon (C) | ≤ 0.08% | Impurity limit |
| Nitrogen (N) | ≤ 0.05% | Impurity limit |
| Hydrogen (H) | ≤ 0.015% | Impurity limit (critical - embrittlement risk) |
| Yttrium (Y) | ≤ 0.005% | Residual limit |
2. Mechanical Properties (ASTM B348, annealed condition)
表格
| Property | Value |
|---|---|
| Tensile strength | ≥ 895 MPa (typically 950–1,100 MPa) |
| Yield strength | ≥ 825 MPa (typically 850–1,000 MPa) |
| Elongation | ≥ 10% (typically 14–18%) |
| Reduction of area | ≥ 25% |
| Hardness | ~320–360 HB (≈ 34–38 HRC) |
| Density | 4.43 g/cm³ (about 56% of steel) |
| Elastic modulus | ~114 GPa |
| Melting range | ~1,600–1,670 °C |
| Service temperature | –250 °C to ~400 °C (long-term) |
After solution treatment + aging (STA), strength can reach 1,100–1,300 MPa - a ~20–30% increase over the annealed condition.
3. Physical Properties
表格
| Property | Value | Notes |
|---|---|---|
| Strength-to-weight ratio | Exceptional | Higher than most steels and aluminum alloys |
| Thermal conductivity | 6.7 W/(m·K) | Low - machining heat concentrates at the tool |
| Thermal expansion | 8.6 × 10⁻⁶/K | Low - good dimensional stability |
| Specific heat | ~560 J/(kg·K) | |
| Biocompatibility | Excellent | Non-toxic, fully accepted by human tissue |
| Corrosion resistance | Outstanding TiO₂ passive film | Seawater, chlorides, oxidizing acids, body fluids |
| Magnetic properties | Non-magnetic | Suitable for MRI-compatible devices |
4. Metallurgical Characteristics
α+β two-phase structure: Aluminum stabilizes the hexagonal α phase; vanadium stabilizes the body-centered cubic β phase (β-transus temperature ≈ 980–1,000 °C).
Heat-treatable: The β phase enables solution + aging treatment for substantial strength gains - a key advantage over commercially pure titanium.
Microstructure control: Processing in the α+β field produces fine duplex (equiaxed α + transformed β) structures with the best balance of strength, ductility, and fatigue resistance.
Sensitivity: Hydrogen pickup must be strictly controlled (welding, pickling, machining coolant); β-phase content increases at elevated temperatures - hot working window must be managed.
5. Manufacturing Process
Melting - Triple vacuum arc remelting (VAR) of sponge titanium + Al-V master alloy for homogeneity
Forging/breakdown - Ingot forged into billets in the β or α+β field
Hot rolling / forging to bar - Rolled or forged to final or near-final diameter (typically 700–950 °C)
Annealing - Mill annealing at 700–850 °C to restore ductility
Cold drawing / centerless grinding (optional) - For precision diameters and surface finishes
Straightening - Rotary or press straightening
Surface treatment - Machining/turning, polishing, or sandblasting
Inspection & testing - UT flaw detection, dimensional checks, tensile testing, PMI, dye penetrant - full MTC (EN 10204 3.1/3.2) supplied
6. Product Forms & Tolerances
表格
| Form | Description | Typical Tolerance |
|---|---|---|
| Hot-rolled bar | As-rolled surface, black/oxidized | h11/h12 |
| Forged bar | Better internal quality, larger diameters | Per agreement |
| Cold-drawn / ground bar | Bright surface, precise dimensions | h8/h9/h10 |
| Peeled/turned bar | Machined surface, removed decarburized/α-case layer | h9/h11 |
| Centerless-ground bar | Mirror or precision finish for machining | h7/h8 |
Surface conditions available: black (as-rolled), pickled, sandblasted, turned/ground, polished.
7. Key Application Areas
Aerospace (largest market)
Aircraft structural components: frames, brackets, fasteners
Engine parts: compressor blades, disks, shafts
Landing gear and actuator components
Helicopter rotor hubs
Medical
Surgical implants: bone screws, plates, intramedullary nails, spinal fixation devices
Dental implant fixtures and abutments
Surgical instruments and tool blanks
(Note: for permanent implants, the ELI version - Grade 23 / Ti-6Al-4V ELI - with lower interstitials is often specified per ASTM F136)
Marine & Offshore
Propeller shafts, underwater fasteners, couplings
Seawater pump components, valve stems
Deep-sea equipment structural parts
Industrial & Energy
Chemical plant shafts, agitators, pump components
High-pressure vessel components
Automotive racing parts (connecting rods, valves)
Sports equipment: bicycle frames, golf club heads, tennis rackets
8. Comparison: GR5 vs. Pure Titanium Bars
表格
| Item | GR2 (TA2) Bar | GR5 (TC4) Bar |
|---|---|---|
| Type | Commercially pure | α+β alloy |
| Tensile strength | ~450–550 MPa | ~950–1,100 MPa |
| Yield strength | ~350 MPa | ~850 MPa |
| Ductility | Higher (ε ≥ 25%) | Moderate (ε ≥ 10–14%) |
| Corrosion resistance | Excellent | Excellent (near-equal) |
| Heat treatment | Annealing only | Solution + aging available |
| Cost | Lower | ~2–3× higher |
| Best for | Chemical equipment, formed parts | Aerospace, medical, high-load parts |
9. Relevant Standards
表格
| Standard | Scope |
|---|---|
| ASTM B348 | Bars and billets - the primary product standard |
| ASTM F67 / F136 | Surgical implant grades (F136 for Ti-6Al-4V ELI) |
| AMS 4928 | Aerospace bar, forging, and ring specification |
| ASME SB348 | Pressure vessel code version |
| GB/T 2965 | Chinese standard for titanium and titanium alloy bars |
| DIN 3.7165 / EN 3.7164 |
European designations
|